India China Australia Malaysia
ASTM A536 Ductile Iron Castings Tensile Requirements NO.
ASTM A536 Ductile Iron Grades
Country
Tensile Requirements 1
Tensile Strength, min, psi
3
Yield Strength, min, psi
2
4
5
Tensile Strength, min, Mpa Yield Strength, min, Mpa
Tensile Strength, min, psi
3
Yield Strength, min, psi
4
5
60,000
65,000
80,000
100,000
120,000
40000
45000
55000
70000
90000
18
12
6.0
3.0
2.0
414
Elongation in 2 in. or 50 mm, min, %
1
2
Grade 60/40/18 Grade 65/45/12 Grade 80/55/06 Grade 100/70/03 Grade 120/90/02
276
448
310
552
379
Tensile Requirements for Special Applications
Tensile Strength, min, Mpa Elongation in 2 in. or 50 mm, min, %
621
70000
80000
42000
50000
60000
10
5
3
290
ISO 9001:2008 Certified
Office: 740-201-8112
483
827
60000 415
Yield Strength, min, Mpa
689
www.mesinc.ne t
485
345
555